Description: OFF-WHITE TALC
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 0.81% | 0.02 | |
| MgO | 30.46% | 0.98 | |
| Al2O3 | 0.51% | 0.01 | |
| SiO2 | 60.91% | 1.32 | |
| Fe2O3 | 1.02% | 0.01 | |
| LOI | 6.30% | n/a | |
| Oxide Weight | 121.66 | ||
| Formula Weight | 129.84 | ||
Cimcoat is an off white yellowstone talc product available in 200 and 325 mesh sizes. Applications include use as a prilling and detackifying agent for ammnonium nitrate fertilizer, seeds and copper sulfate granules. It can be used as a carrier for insecticides, herbicides and time release fertilizers. It is also used in traffic paint, color insenstitive primers and applications where viscosity build and anti-settling properties are needed at an affordable price.
Physical Properties:
TAPPI Brightness GEB (LASTM-14) 67-75
Hegman Fineness (LASTM-17) 3.0
Oil Absorption, SRO (LASTM-18) 3.0
Specific Gravity (LASTM-06) 2.8
Surface Area, m2/gm (BET-N2) 6.6
pH, 10% slurry (LASTM-05) 9.5
Tapped Density, lbs/ft3 (LASTM-13) 54
Loose Density, lbs/ft3 (LASTM-12) 21
Bulking Value, lbs/gal 23.3
Average Moisture (LASTM-04) .5%
Median Diameter, microns (LASTM-02) 6.2
Mineralogy:
Talc 93.5
Dolomite 3.5
Quartz 1.5
Calcite .5
Chlorite 1.0
*LASTM - Luzenac America Standard Test Method
Luzenac America, Inc, 9000 East Nichols Ave, Englewood, CO 80112.
| Typecodes |
Flux Source
Materials that source Na2O, K2O, Li2O, CaO, MgO and other fluxes but are not feldspars or frits. Remember that materials can be flux sources but also perform many other roles. For example, talc is a flux in high temperature glazes, but a matting agent in low temperatures ones. It can also be a flux, a filler and an expansion increaser in bodies. |
| Hazards |
Talc Hazards Overview
Talc is invaluable in the ceramics industry, it is used as a glaze and body ingredient and as a parting a release agent in various processes. Is it safe? |
| Materials |
Talc
A source of MgO for ceramic glazes, a flux or thermal expansion additive in clay bodies, also used in the manufacture of cordierite. |