Pyrofrac 1655

Oxide Analysis Formula Tolerance
K2O 0.45% 0.04
Na2O 0.45% 0.05
TiO2 0.40% 0.04
Al2O3 13.50% 1.00
SiO2 79.00% 9.93
Fe2O3 1.00% 0.05
Cl 5.20%n/a
Oxide Weight 716.27
Formula Weight 755.56

Notes

Used in structural clay coatings, refractory formulations, whiteware ceramics, art pottery to
increase refractoriness, reduce shrinkage, and widen firing range.
This material is made by crushing & screening of selectively mined andalusite/pyrophyllite/sericite ores
with heavy media separation.

Related Information

Links

Materials Andalusite
Materials Pyrophyllite
A refractory aluminum silicate mineral often used in clay body recipes to lower thermal expansion, control fired maturity, mullite development catalyst, etc.
Materials Alkatrol
Materials Pyrofrac
Materials Seriphyl

Data

Bulk Density lbs/cu. ft. (Packed) 65
Pyrometric Cone Equivalent 20
Sieve Analysis Dry +50 mesh: 0.1 +70 mesh: 0.1 +100 mesh: 1.1 +200 mesh: 8.6 +325 mesh: 21.0
Density (Specific Gravity) 2.6
By Tony Hansen