1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

Midstone

Description: Plainsman Native Clay

Oxide Analysis Formula Tolerance
BaO 0.32% 0.01
CaO 0.23% 0.02
K2O 2.59% 0.16
MgO 0.65% 0.10
Na2O 0.06% 0.01
TiO2 0.68% 0.05
Al2O3 17.19% 1.00
P2O5 0.15% 0.01
SiO2 70.37% 6.95
Fe2O3 1.26% 0.05
MnO 0.01% -
LOI 6.49%n/a
Oxide Weight 554.86
Formula Weight 593.37

Notes

A unique fine grained, clean material, vitrifying and reaching very high strength at cone 8. It is well balanced and of medium plasticity and suitable as the main constituent for mid-temperature bodies and to promote vitrification in the higher ranges without adding dark color. This material is balanced enough to use by it self for pottery.

Fired Temperature, Cone 3 4 5 6 7 8
--------------------------------------
Fired Shrinkage: 4.5% 4.8% 5.2% 5.6% 6.1% 6.0%
Absorption: 6.0% 5.0% 3.8% 2.4% 1.4% 1.0%
Fired Strength:
(lbs/ square inch) 7000 9000 10700 11600 12200

Sieve Analysis Wet Washed
(Root of 2 series) +35 +48 +65 +100 +150# +200 +325
--------------------------------------------
0.0% 0.1 0.4% 1.2% 2.0% 4.1% 11.8%

Texture: Smooth
Plastic Index (1-10): 6
Green Strength (lbs/sqaure inch): 1050
Dry shrinkage: 6.0
Dried density: 2.03
PCE: 23

Related Information

What does Goldart look like if you fire it by itself?


Goldart fired bars

This picture has its own page with more detail, click here to see it.

Goldart (left) compared to Plainsman Midstone (right). Goldart is a buff and vitreous stoneware at cone 10R. These are fired at cone 7, 8, 10 oxidation and 10 reduction (bottom to top). Soluble salts in the Goldart impart a darker coloration to the reduction fired bar). The Midstone has some coarser particles that make for larger speckles in reduction.

Links

Typecodes Clay Other
Clays that are not kaolins, ball clays or bentonites. For example, stoneware clays are mixtures of all of the above plus quartz, feldspar, mica and other minerals. There are also many clays that have high plasticity like bentonite but are much different mineralogically.

Data

Frit Softening Point PCE 23

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy