From page 144 in Mastering Glazes.
Step 1 is to provide time for all remaining or residual water in glaze and clay to evaporate. However 220F may not be high enough, 250F is usually needed (and will not fracture ware). This segment should also have a hold, at least 60 minutes.
| Step | °C | °F | Hold | Time | |
|---|---|---|---|---|---|
| 1 | 55°C/hr to 105C | 99°F/hr to 221F | 0 | 1:58 | |
| 2 | 200°C/hr to 1080C | 360°F/hr to 1976F | 0 | 6:51 | |
| 3 | 85°C/hr to 1200C | 153°F/hr to 2192F | 15min | 8:30 | Confirm with self supporting cone |
| 4 | 275°C/hr to 1000C | 495°F/hr to 1832F | 0 | 9:14 | |
| 5 | 70°C/hr to 760C | 126°F/hr to 1400F | 0 | 12:40 |
| Recipes |
MGBase7 - Raspberry Cone 6 (Mastering Glazes)
From page 102 in Mastering Glazes book |
| Recipes |
MGBase2 - High Calcium Semimatte 2 (Mastering Glazes)
Base from Mastering Glazes book page 89 |
| Recipes |
MGBase1 - High Calcium Semimatte 1 (Mastering Glazes)
From page 86 of Mastering Glazes book |
| Recipes |
MGBase3 - General Purpose Glossy Base 1 (Mastering Glazes)
From page 92 in Mastering Glazes book |
| Recipes |
MGBase4 - Glossy Base 2 Cone 6 (Mastering Glazes)
From page 96 in Mastering Glazes book |
| Recipes |
MGBase5 - Glossy Clear Liner Cone 6 (Mastering Glazes)
From page 97 of Mastering Glazes book |
| Recipes |
MGBase6 - Zinc Semimatte Glossy Base Cone 6
From page 98 of Mastering Glazes book |
| Recipes |
MGBase8 - Waxwing Brown Cone 6 (Mastering Glazes)
From page 104 in Mastering Glazes book |
| Recipes |
MGBase9 - Waterfall Brown Cone 6 (Mastering Glazes)
From page 106 of Mastering Glazes book |
| Firing Schedules |
Plainsman Cone 6 Drop-and-hold, Slow Cool
350F/hr to 2100F, 108/hr to 2200, hold 10 minutes, fastdrop to 2100, hold 30 minutes, 150/hr to 1400 |
| Firing Schedules | Plainsman Cone 5 Drop-and-Hold Slow-Cool |
| Oxides | Sm2O3 - |
| Typecodes | Oxidation Firing |
![]() PayPal | No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me. |
| By Tony Hansen Follow me on ![]() | ![]() |
Buy me a coffee and we can talk