Description: ALUMINA
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 0.02% | - | |
| Na2O | 0.10% | - | |
| Al2O3 | 99.70% | 1.00 | |
| SiO2 | 0.02% | - | |
| Fe2O3 | 0.02% | - | |
| LOI | 0.10% | n/a | |
| Oxide Weight | 102.16 | ||
| Formula Weight | 102.27 | ||
This is an intermediate soda, medium crystalline 3rd generation calcined
alumina.
WRA A-17 A-16
Ultimate crystal size d50-Eppendorf, microns: 2.5-3.2 3.0-3.5 .3-.5
Al2O3 99.5+ 99.5+
SiO2 .02 for A17, .01 for A16
Fe2O3 .01 for all
Na2O3 .08 for A17 and A16
Specific surface area: BET, m2/g .5-.8 3 3-7
Aggregate size, % for WRA: >150 micron 1-10, >63 " 60-80, >40 70-95
Grinding time, Hrs: 4 for A17, 16 for A16
Green density, g/cc: 2.15 for A16, 2.5 for A17
Fired density, g/cc: 3.88 for A16, 3.75 for A17
From Aluminum Company of America
1501 Alcoa Building
Chemicals Division
Pittsburg, PA 15219
| Typecodes |
Alumina
Alumina products |
| Glossary |
Calcination
Calcining is simply firing a ceramic material to create a powder of new physical properties. Often it is done to kill the plasticity or burn away the hydrates, carbonates, sulfates of a clay or refractory material. |