Description: HIGHLY REFINED WHITE HECTORITE

Oxide Analysis Formula Tolerance
CaO 2.96% 0.07
K2O 0.12% -
Li2O 1.50% 0.07
MgO 24.90% 0.81
Na2O 2.43% 0.05
TiO2 0.18% -
Al2O3 0.93% 0.01
SiO2 46.20% 1.01
Fe2O3 0.78% 0.01
LOI 20.00%n/a
Oxide Weight 105.07
Formula Weight 131.33

Notes

A highly refined white hectorite that is four to five times more efficient than other purified clays. A plasticizing agent for non-plastic alumina or zirconia bodies.

Specific Gravity: 2.5
pH (5% dispersion): 9.5-10.5
C.E.C. (meq/100g): 124
Dry Brightness (Green Filter): 86
Color: White
% Moisture Content: 10% Max.
Brookfield Viscosity (60 rpm @ 5% solids): 8210cps

Related Information

Links

Typecodes Clay Other
Clays that are not kaolins, ball clays or bentonites. For example, stoneware clays are mixtures of all of the above plus quartz, feldspar, mica and other minerals. There are also many clays that have high plasticity like bentonite but are much different mineralogically.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy