Description: FINE WHITE CALCIUM HECTORITE

Oxide Analysis Formula Tolerance
CaO 4.04% 0.12
K2O 0.33% 0.01
Li2O 1.50% 0.09
MgO 17.90% 0.77
Na2O 0.50% 0.01
TiO2 0.20% -
Al2O3 4.21% 0.07
SiO2 44.10% 1.27
Fe2O3 1.36% 0.01
LOI 25.80%n/a
Oxide Weight 128.25
Formula Weight 172.84

Notes

Finely ground, white, calcium hectorite clay. Used as a binder in extruded tile to increase green strength with minimum increases in viscosity.

Specific Gravity: 2.5
pH (5% dispersion): 8.5-9.5
C.E.C. (meq/100g): 104
Dry Brightness (Green Filter): 71
Color: White
% Moisture Content: 10% Max.
Brookfield Viscosity (60 rpm @ 5% solids): 24cps

Related Information

Links

Typecodes Clay Other
Clays that are not kaolins, ball clays or bentonites. For example, stoneware clays are mixtures of all of the above plus quartz, feldspar, mica and other minerals. There are also many clays that have high plasticity like bentonite but are much different mineralogically.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy