Description: FINE GROUND SODIUM HECTORITE

Oxide Analysis Formula Tolerance
CaO 6.74% 0.17
K2O 0.73% 0.01
Li2O 1.50% 0.07
MgO 19.00% 0.69
Na2O 2.35% 0.06
TiO2 0.27% -
Al2O3 3.81% 0.05
SiO2 43.40% 1.05
Fe2O3 1.55% 0.01
LOI 20.60%n/a
Oxide Weight 115.40
Formula Weight 145.34

Notes

Finely ground, white, sodium hectorite clay exhibiting high cation exchange capacity. Used as a binder and plasticizer in wall and floor tile. Exhibits excellent increases in green strength.

Specific Gravity: 2.5
pH (5% dispersion): 9.5-10.5
C.E.C. (meq/100g): 100
Dry Brightness (Green Filter): 70
Color: White
% Moisture Content: 10% Max.
Brookfield Viscosity (60 rpm @ 5% solids): 2380cps

Related Information

Links

Typecodes Clay Other
Clays that are not kaolins, ball clays or bentonites. For example, stoneware clays are mixtures of all of the above plus quartz, feldspar, mica and other minerals. There are also many clays that have high plasticity like bentonite but are much different mineralogically.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy