1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

vol351cer

Description: FINE GROUND SODIUM BENTONITE

Oxide Analysis Formula Tolerance
CaO 1.51% 0.16
K2O 0.85% 0.05
MgO 3.85% 0.56
Na2O 2.40% 0.23
TiO2 0.17% 0.01
Al2O3 13.50% 0.78
SiO2 68.60% 6.71
Fe2O3 1.71% 0.06
LOI 7.40%n/a
Oxide Weight 544.06
Formula Weight 587.54

Notes

A finely ground, white, sodium bentonite that exhibits low viscosity. Used as a binder in extruded bodies to add plasticity with no increases in viscosity.

Specific Gravity: 2.5
pH (5% dispersion): 8.5-9.5
C.E.C. (meq/100g): 80
Dry Brightness (Green Filter): 81
Color: White
% Moisture Content: 10% Max.
Brookfield Viscosity (60 rpm @ 5% solids): 28cps

Related Information

Links

Materials Bentonite
Bentonite can make a clay body instantly plastic, only 2-3% can have a big effect. It also suspends slurries so they don't settle out and slows down drying.
Typecodes Clay Other
Clays that are not kaolins, ball clays or bentonites. For example, stoneware clays are mixtures of all of the above plus quartz, feldspar, mica and other minerals. There are also many clays that have high plasticity like bentonite but are much different mineralogically.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy