SP BWS Ball Clay

Description: WBB Devon Ball Clay Group 2

Oxide Analysis Formula Tolerance
CaO 0.20% 0.01
K2O 1.40% 0.04
MgO 0.40% 0.03
Na2O 0.10% -
TiO2 0.80% 0.03
Al2O3 33.80% 1.00
SiO2 47.60% 2.39
Fe2O3 1.20% 0.02
LOI 14.50%n/a
C 3.00%n/a
Oxide Weight 258.02
Formula Weight 312.75

Notes

Particle Size (e.s.d.)
125 microns - 1.00
10 microns - 97
2 microns - 84
1 microns - 75
Modulus of Rupture at 110C
Mn/M2 - 4.8
lbf/in2 - 700
Defloculant Required - (3:1 Na2SiO3(C.100):Na2CO3) - 0.5
Water Absorption
1120C - 9.0
1220C - 1.50
Shrinkage Dry to Fired
1120C - 14.50
1220C - 18.00
Reflectance 464nm
1120C - 80
1220C - 73
Refractoriness
Cone - 33, 1730C

Related Information

Links

Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.