Description: WBB Devon Ball Clay Group 4

Oxide Analysis Formula Tolerance
CaO 0.20% 0.02
K2O 2.20% 0.10
MgO 0.30% 0.03
Na2O 0.30% 0.02
TiO2 1.40% 0.08
Al2O3 23.40% 1.00
SiO2 64.90% 4.71
Fe2O3 0.80% 0.02
LOI 6.50%n/a
C 0.20%n/a
Oxide Weight 407.56
Formula Weight 436.83

Notes

Particle Size (e.s.d.)
125 microns - 0.60
10 microns - 96
2 microns - 75
1 microns - 65
Modulus of Rupture at 110C
Mn/M2 - 4.6
lbf/in2 - 670
Defloculant Required - (3:1 Na2SiO3(C.100):Na2CO3) - 0.5
Water Absorption
1120C - 1.0
1220C - 0.50
Shrinkage Dry to Fired
1120C - 11.50
1220C - 12.50
Reflectance 464nm
1120C - 64
1220C - 47
Refractoriness
Cone - 31, 1690C

Related Information

Links

Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy