1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

Principio Stoneware

Description: Legacy stoneware from United Clay Mines

Oxide Analysis Formula Tolerance
SiO2 59.40% 4.03
Al2O3 25.00% 1.00
Fe2O3 2.80% 0.07
TiO2 0.90% 0.05
CaO 0.30% 0.02
MgO 0.20% 0.02
K2O 2.10% 0.09
Na2O 0.70% 0.05
LOI 8.60%n/a
Oxide Weight 372.91
Formula Weight 408.00

Related Information

Links

Typecodes Stoneware Clay
These materials generally contain bentonite, ball clay, kaolin, feldspar, mica, quartz and some iron impurities. They can often be used as a body with few additives.

Data

% < 0.5 microns 52%
Drying Shrinkage n/a
Firing Shrinkage 19% at cone 9
Water absorption 0% at cone 9
Dry M.O.R. (50% Silica) 820 psi

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy