Alternate Names: PotteryCrafts Frit 3124
Description: This is actually Ferro Frit 3124
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 14.10% | 0.70 | |
| K2O | 0.70% | 0.02 | |
| Na2O | 6.30% | 0.28 | |
| B2O3 | 13.70% | 0.55 | |
| Al2O3 | 9.90% | 0.27 | |
| SiO2 | 55.30% | 2.55 | |
| Oxide Weight | 277.48 | ||
| Formula Weight | 277.48 | ||
| Materials |
Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot. |
| Materials |
Ferro Frit 3124
A commonly available calcium borosilicate frit. It is glaze-like, needing only a kaolin addition to create a low-temperature glossy glaze. |
| Typecodes |
Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types. |
| Co-efficient of Linear Expansion | 7.9 |
|---|---|
| Frit Melting Range (C) | 1000-1020 |