Pemco Frit Pb-2G30

Alternate Names: Frit Pb2G30

Description: Low lead calcium frit

Oxide Analysis Formula Tolerance
CaO 9.90% 0.56
K2O 1.60% 0.05
Na2O 2.50% 0.13
PbO 18.10% 0.26
B2O3 5.50% 0.25
Al2O3 6.10% 0.19
SiO2 56.30% 2.98
Oxide Weight 317.59
Formula Weight 317.59

Notes

Dinnerware glaze component - Cone 1 to 4.
Used the same as Pb-349, excellent for underglaze colors.

Related Information

Links

Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Materials Ferro Frit 349
Typecodes Leaded Frit
Frits can contain 1% or 80% PbO so this category can be misleading, check the chemistry to find out.
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.

Data

Co-efficient of Linear Expansion 6.00
Co-efficient of Linear Expansion 6.0 x 10-6 (50-450C)
Frit Softening Point 1570F
Frit Melting Range (C) 1520-1650F
I.F.P. (celsius) 600C

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy