Pemco Frit Pb-197

Alternate Names: Frit Pb167

Description: Zinc bearing lead frit for all-fritted glaze cone 04-6

Oxide Analysis Formula Tolerance
CaO 5.90% 0.29
K2O 2.40% 0.07
Na2O 4.00% 0.18
PbO 11.30% 0.14
ZnO 9.50% 0.32
B2O3 6.50% 0.26
Al2O3 7.40% 0.20
SiO2 53.00% 2.43
Oxide Weight 275.86
Formula Weight 275.86

Notes

When 5% alumina and 10% clay are added, a good base for chrome-alumina pinks results.

Related Information

Links

Materials Ferro Frit 3563
Materials Fusion Frit FZ-9
Materials Pemco Frit Pb-704
Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Materials Ferro Frit 3552
Materials Hommel Frit 419
Typecodes Leaded Frit
Frits can contain 1% or 80% PbO so this category can be misleading, check the chemistry to find out.
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.

Data

Co-efficient of Linear Expansion 7.20
Co-efficient of Linear Expansion 7.2 x 10-6 (50-450C)
Frit Softening Point 1550F
Frit Melting Range (C) 1500-1600F
I.F.P. (celsius) 610C

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy