1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

Pemco Frit Pb-1492

Alternate Names: Frit Pb1492

Description: LEADED FRIT

Oxide Analysis Formula Tolerance
CaO 8.90% 0.44
K2O 1.60% 0.05
Li2O 0.70% 0.06
MgO 1.40% 0.10
Na2O 2.00% 0.09
PbO 14.10% 0.17
SrO 3.60% 0.10
B2O3 9.30% 0.37
Al2O3 6.20% 0.17
SiO2 52.20% 2.39
Oxide Weight 274.70
Formula Weight 274.70

Notes

Particularly suited for wollastonite bodies in a range of Cone 04 through Cone 2. Can be used alone or in partially-fritted glazes.

Related Information

Links

Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Typecodes Leaded Frit
Frits can contain 1% or 80% PbO so this category can be misleading, check the chemistry to find out.
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.

Data

Co-efficient of Linear Expansion 6.7 x 10-6 (50-450C)
Frit Softening Point 1500F
Frit Melting Range (C) 1470-1580F
I.F.P. (celsius) 610C

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy