Pemco Frit Pb-1114

Alternate Names: Frit Pb1114

Description: Calcium borosilite medium lead frit for cone 08-04 glazes

Oxide Analysis Formula Tolerance
CaO 9.80% 0.48
K2O 1.40% 0.04
Na2O 1.90% 0.08
PbO 31.60% 0.39
B2O3 11.10% 0.44
Al2O3 3.50% 0.09
SiO2 40.70% 1.87
Oxide Weight 276.42
Formula Weight 276.42

Notes

Good for low temperature, clear and colored glazes. Can be blended with Pb-349, Pb-1241 or Pb-1421 for intermediate temperatures.

Related Information

Links

Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Materials General Frit GF-20
Materials Hommel Frit 4GF48B
Typecodes Leaded Frit
Frits can contain 1% or 80% PbO so this category can be misleading, check the chemistry to find out.
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.

Data

Co-efficient of Linear Expansion 7.00
Co-efficient of Linear Expansion 7.0 x 10-6 (40-450C)
Frit Softening Point 1400F
Frit Melting Range (C) 1350-1500F
I.F.P. (celsius) 600C

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy