Pemco Frit Pb-106

Alternate Names: Frit Pb106

Description: Lead high calcium frit for dinnerware glazes

Oxide Analysis Formula Tolerance
CaO 18.00% 0.78
K2O 1.60% 0.04
Na2O 1.80% 0.07
PbO 10.10% 0.11
B2O3 19.50% 0.68
Al2O3 3.40% 0.08
SiO2 45.60% 1.84
Oxide Weight 242.65
Formula Weight 242.65

Related Information

Links

Materials Pemco Frit P-25
Materials Hommel Frit 25
Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Typecodes Leaded Frit
Frits can contain 1% or 80% PbO so this category can be misleading, check the chemistry to find out.
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.

Data

Co-efficient of Linear Expansion 7.80
Co-efficient of Linear Expansion 7.8 x 10-6 (50-450C)
Frit Softening Point 1680F
Frit Melting Range (C) 1650-1730F
I.F.P. (celsius) 658C

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy