Pemco Frit Pb-1038

Alternate Names: Frit Pb1038

Description: All-fritted base for chome-alumina pink stains

Oxide Analysis Formula Tolerance
K2O 0.30% 0.01
Na2O 2.70% 0.13
PbO 43.50% 0.58
ZnO 7.60% 0.28
B2O3 5.00% 0.21
Al2O3 5.00% 0.15
SiO2 35.90% 1.78
Oxide Weight 298.51
Formula Weight 298.51

Notes

For cone 06-02. May be blended with Pb-197 for intermediate temperatures.

Related Information

Links

Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Materials Hommel Frit 634
Typecodes Leaded Frit
Frits can contain 1% or 80% PbO so this category can be misleading, check the chemistry to find out.
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.

Data

Co-efficient of Linear Expansion 6.8 x 10-6 (40-450C)
Frit Melting Range (C) 1300-1400F
I.F.P. (celsius) 525C

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy