Alternate Names: Frit 786, Frit P786
Description: Leadless all-fritted glaze
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 11.50% | 0.58 | |
| K2O | 3.00% | 0.09 | |
| Na2O | 2.00% | 0.09 | |
| SrO | 8.70% | 0.24 | |
| B2O3 | 8.80% | 0.36 | |
| Al2O3 | 6.80% | 0.19 | |
| SiO2 | 59.20% | 2.79 | |
| Oxide Weight | 283.23 | ||
| Formula Weight | 283.23 | ||
Used for vitreous and semi-vitreous dinnerwre and artware. Same as Pb-349 with strontia replacing lead. Fires cone 02-8.
| Materials |
Pemco Frit Pb-349
|
| Materials |
Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot. |
| Materials |
Hommel Frit 630
|
| Typecodes |
Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types. |
| Co-efficient of Linear Expansion | 7.2 x 10-6 (50-450C) |
|---|---|
| Frit Melting Range (C) | 1640-1910F |