Pemco Frit P-318

Alternate Names: Frit 318, Frit P318

Description: Leadless high barium zero alumina borosilicate flux

Oxide Analysis Formula Tolerance
BaO 41.90% 1.00
B2O3 19.90% 1.05
SiO2 38.20% 2.33
Oxide Weight 365.87
Formula Weight 365.87

Notes

Used in partially-fritted matte and art glazes.

Related Information

Links

Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Materials Hommel Frit 385
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.

Data

Co-efficient of Linear Expansion 7.0 x 10-6 (50-450C)
Frit Melting Range (C) 1650-1800F
I.F.P. (celsius) 650C

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy