Oxide Analysis Formula Tolerance
CaO 12.50% 0.50
K2O 3.40% 0.08
MgO 3.20% 0.18
Na2O 6.60% 0.24
B2O3 12.20% 0.39
Al2O3 7.10% 0.16
SiO2 55.10% 2.06
Oxide Weight 225.06
Formula Weight 225.06

Notes

Comment: Used as a component of a vellum-type matte glaze firing at Cone 3 to Cone 5. This glaze is good on dinnerware because it will not knife-mark in general usage.

Related Information

Links

Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.

Data

Co-efficient of Linear Expansion 9.3x10-6 (50-450C)
Frit Melting Range (C) 1420-1520F
I.F.P. (celsius) 607C

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy