1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

Omr Ball Clay

Description: Tennessee Ball Clay

Oxide Analysis Formula Tolerance
CaO 0.50% 0.03
K2O 0.70% 0.03
MgO 0.60% 0.06
Na2O 0.10% 0.01
TiO2 1.20% 0.06
Al2O3 27.40% 1.00
SiO2 57.50% 3.56
Fe2O3 2.60% 0.06
LOI 9.50%n/a
C 0.20%n/a
Oxide Weight 337.27
Formula Weight 373.50

Notes

Particle Size (e.s.d.)
125 microns - 0.2
20 microns - 97
2 microns - 87
.5 microns - 72
Modulus of Rupture at 110C
Mn/M2 - 15.5
lbf/in2 - 2250
Water Absorption
1120C - 15.0
1220C - 0.5
Shrinkage Dry to Fired
1120C - 8.0
1220C - 12.0
Refractoriness
Cone - 32, 1710C

Related Information

Links

Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy