Old Hickory No 6 Ball Clay

Description: Legacy ball clay

Oxide Analysis Formula Tolerance
SiO2 50.10% 2.58
Al2O3 33.00% 1.00
Fe2O3 0.90% 0.02
TiO2 1.30% 0.05
CaO 1.40% 0.08
MgO 0.30% 0.02
K2O 0.40% 0.01
Na2O 0.70% 0.03
LOI 12.00%n/a
Oxide Weight 272.31
Formula Weight 309.44

Related Information

Links

Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.

Data

% < 0.5 microns 43%
Drying Shrinkage 8.0%
Firing Shrinkage Cone 9: 8.0%
Water absorption Cone 9: 0%
Dry M.O.R. (50% Silica) 500 psi

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy