No. 1 Glaze Ball Clay

Alternate Names: Glaze #1, #1 Glaze Clay

Description: Kentucky Ball Clay, Glaze #1, Glaze Number 1, Glaze No 1

Oxide Analysis Formula Tolerance
CaO 0.10% 0.01
K2O 0.30% 0.01
MgO 0.30% 0.03
Na2O 0.10% 0.01
TiO2 2.40% 0.10
Al2O3 29.40% 1.00
SiO2 56.30% 3.25
Fe2O3 0.90% 0.02
LOI 9.90%n/a
Oxide Weight 311.55
Formula Weight 345.78

Notes

This is a high alumina, low iron ball clay (typical ball clays can be less than 25% alumina). As its name suggests, this works well as a suspender and hardener in glazes, especially for whites and transparents where the cleanest possible materials are needed. The Old Hickory No. 5 ball clay is a similar material. Use less than 20% (in glazes having no other clay materials) or excessive gelling could occur.

Crude Color: White
Dry M.O.R. (psi 50% clay/50% flint, cast bars): 400
Wet Sieve Residue, +200 mesh (%): 0.20
Water of Plasticity (%): 32
Linear Dry Shrinkage (%): 6.2
Solubles Sulfates (ppm): 183
Filtration (ml): 26
Specific Surface Area (sq meters per gram): 18.0
CEC/MBI (meq/100 ml): 9.5
pH: 5.7
PCE: 32

Firing Shrinkage (%) Cone 04: 4.1 Cone 3: 5.5 Cone 11: 6.8
Absorption (%) 15.9 12.0 5.4

Particle Size (% finer than):
50 microns: 100
20: 98
10: 95
5: 82
1: 55
0.5: 44

Related Information

The ball clay you use to suspend your glaze is important!


Running behavior of two glaze slurries

This picture has its own page with more detail, click here to see it.

I poured 4 teaspoons of two glazes onto a non-absorbent butcher’s board and let them sit for a minute, then inclined the board. The one on the right employs Gleason Ball clay, the left one has Old Hickory #5 ball clay. Neither has any rheology modifier additions. The one on the right has settled and, on incline of the board, the watery upper is running off. The other has gelled and the whole thing is running downward slowly. Below that you can see where I have begun to sponge them off, the one on the right is sticky. The most amazing thing about this: This difference appears despite the fact that there is only 7% ball clay in this heavily fritted recipe.

Links

Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.
Materials No. 5 Ball Clay
URLs http://oldhickoryclay.com/products/kentucky-clays/no-1-glaze/
No. 1 Glaze ball clay data sheet

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy