Mullite Fused Dense

Description: ELTRO FUSED MULLITE

Oxide Analysis Formula Tolerance
CaO 0.05% -
K2O 0.15% -
MgO 0.05% -
Na2O 0.15% -
TiO2 0.01% -
Al2O3 76.30% 1.00
SiO2 23.30% 0.52
Fe2O3 0.05% -
Oxide Weight 133.76
Formula Weight 133.76

Notes

Particle Size: 0.7-1.5mm
Free iron grains: .02% max
Grain porosity: 2%
Bulk density: 2.09 g/cm3
Refractoriness: 1900C

Also available in sizes: 0.125-0.25mm, 0.25-0.5mm, 0.5-1.0mm for precision metal casting industry and -45 micron for use as a face coat.

Related Information

Links

Typecodes Aggregate
Granular materials intended to impart raw and fired structural strength or thermal expansion properties to bodies or deliver special speckling effects in glazes.

Data

Density (Specific Gravity) 3.14

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy