1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

Milwhite Bentonite B

Description: WHITE FIRING BENTONITE

Oxide Analysis Formula Tolerance
K2O 0.69% 0.07
Na2O 0.67% 0.10
Fe2O3 0.74% 0.04
CaO 2.20% 0.35
MgO 2.21% 0.49
Al2O3 22.60% 1.98
SiO2 62.54% 9.28
LOI 8.40%n/a
Oxide Weight 816.95
Formula Weight 891.87

Notes

From Milwhite Inc., Box 15038, HOUSTON, TX 77220 Phone 713-675-0961 FAX
713-675-4162

Is is a natural select calcium montmorillonite.
Specific Gravity: 2.5-2.75
Moisture as produced: 12-14%
pH: 7.3-7.7
Color: Off White raw (Beige/White at 1800F)
On 100 mesh wet: .1
On 200 mesh wet: 3.0
Bulk Density: 37 lbs/ft3
Packed Density: 58
CEC: 45
Swelling Index (ml/2 gm): 3.0

It is available in 50 lb or 2000 lbs bulk bags.

Related Information

Links

Materials Bentonite
Bentonite can make a clay body instantly plastic, only 2-3% can have a big effect. It also suspends slurries so they don't settle out and slows down drying.
Typecodes Clay Other
Clays that are not kaolins, ball clays or bentonites. For example, stoneware clays are mixtures of all of the above plus quartz, feldspar, mica and other minerals. There are also many clays that have high plasticity like bentonite but are much different mineralogically.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.