Martin #5 Ball Clay

Alternate Names: Martin#5, Wade Martin Ball Clay

Description: Tennessee Ball Clay

Oxide Analysis Formula Tolerance
CaO 0.30% 0.02
K2O 1.00% 0.04
MgO 0.40% 0.04
Na2O 0.30% 0.02
TiO2 1.20% 0.05
Al2O3 27.90% 1.00
SiO2 55.20% 3.36
Fe2O3 1.10% 0.03
LOI 12.60%n/a
Oxide Weight 319.53
Formula Weight 365.59

Notes

A coarse-grained, fast casting ball clay used exclusively in casting bodies. Applications include sanitaryware, artware and dinnerware.

Shipped from Whitlock, TN

Water of Plasticity: 28.0%
% Dry Shrinkage: 4.5
Dry M.O.R., psi:* 420
pH: 5.0
C.E.C., meq/100g: 5.5
Soluble sulfur:** Low

Cone 5 10
----
Total Shrinkage: 9.5% 11.0%
Absorption: 12.5% 5.5%

P.C.E.: 31

Particle Size, Microns: 20 10 5 2 1 0.5 0.2
90% 82% 73% 56% 43% 30% 15%

*Modulus of Rupture Specimens: De-aired, extruded, 50% ball clay, 50% flint
**Low-trace to 150, Med-150-400, High-450+

Related Information

Links

Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy