KY-5 Bond Ball Clay

Description: Kentucky Ball Clay

Oxide Analysis Formula Tolerance
CaO 0.30% 0.02
K2O 0.80% 0.03
MgO 0.50% 0.04
Na2O 0.30% 0.02
TiO2 1.90% 0.08
Al2O3 29.50% 1.00
SiO2 54.80% 3.15
Fe2O3 0.70% 0.02
LOI 11.20%n/a
Oxide Weight 307.04
Formula Weight 345.76

Notes

An intermediate-grained high alumina ball clay. Used primarily in the refractory and abrasives industries.


Shipped from Mayfield, KY

Water of Plasticity: 34.0%
% Dry Shrinkage: 6.0
Dry M.O.R., psi:* 540
pH: 4.1
C.E.C., meq/100g: 8.5
Soluble sulfur:** Low

Cone 5 10
----
Total Shrinkage: 12.5% 16.0%
Absorption: 12.5% 4.5%

P.C.E.: 32

Particle Size, Microns: 20 10 5 2 1 0.5 0.2
99% 96% 92% 83% 72% 57% 29%

*Modulus of Rupture Specimens: De-aired, extruded, 50% ball clay, 50% flint
**Low-trace to 150, Med-150-400, High-450+

Related Information

Links

Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy