Oxide Analysis Formula Tolerance
CaO 0.20% 0.01
K2O 1.10% 0.05
MgO 0.40% 0.04
Na2O 0.20% 0.01
TiO2 1.60% 0.08
Al2O3 24.90% 1.00
SiO2 60.90% 4.15
Fe2O3 1.00% 0.03
LOI 9.20%n/a
Oxide Weight 369.90
Formula Weight 407.38

Notes

An intermediate-grained Ball Clay with very good plasticity and strength. KTS-2 can be used in both casting and plastic formed bodies. It is also supplied in a clay-water slurry form for use by the sanitaryware and artware industries.

Physical Properties
===================
Water of Plasticity: 32.6%
% Dry Shrinkage: 5.4
Dry M.O.R. (50:50 ball clay:silica, psi): 580
pH: 4.3
M.B.I. (meq/100g): 6.9
Specific Surface Area (sq-meter/g): 19.0
Soluble sulphur SO4: Medium

P.C.E.: 31

Particle Size, Microns: 20 10 5 2 1 0.5
(% finer than) 93% 86% 73% 58% 46% 35%

Fired Properties
================
Cone 5 10
Total Shrinkage: 11.5% 14.6%
Absorption: 12.2% 5.5%

*This info is from a data sheet from Jan 2013

Related Information

Links

Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy