Kentucky #5 Bond

Description: Kentucky Ball Clay

Oxide Analysis Formula Tolerance
CaO 0.40% 0.02
K2O 1.20% 0.04
MgO 0.40% 0.03
Na2O 0.20% 0.01
TiO2 1.80% 0.08
Al2O3 29.70% 1.00
SiO2 55.40% 3.17
Fe2O3 1.00% 0.02
LOI 7.10%n/a
Oxide Weight 309.43
Formula Weight 333.08

Notes

An intermediate-grained,high-alumina ball clay used primarily in the refractories and abrasives industries.

Physical Properties
===================
Water of Plasticity*: 37.0%
% Dry Shrinkage*: 6.5
Dry M.O.R., psi:* 825
pH: 4.4
C.E.C., meq/100g: 11.0
Specific Surface Area, sq metre/g: 24.4
Soluble sulfur+: Low

P.C.E.: 32

Particle Size, Microns: 20 10 5 2 1 0.5 0.2
(% finer than) 99% 97% 93% 81% 72% 56% 35%

Fired Properties
================
Cone 5 10
----
Total Shrinkage: 13.0% 14.5%
Absorption: 10.0% 1.0%

------------------
*Extruded, 50% ball clay, 50% flint
+Low-trace to 150, Med-150-400, High-450+
**50% Clay, 50% Nepheline Syenite

Related Information

Links

Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy