K&T Special

Alternate Names: Kentucky Special Ball Clay

Description: Kentucky Ball Clay

Oxide Analysis Formula Tolerance
CaO 0.30% 0.02
K2O 0.90% 0.04
MgO 0.50% 0.05
Na2O 0.20% 0.01
TiO2 1.50% 0.07
Al2O3 27.40% 1.00
SiO2 53.30% 3.30
Fe2O3 1.10% 0.03
LOI 14.80%n/a
Oxide Weight 317.17
Formula Weight 372.26

Notes

Water of Plasticity: 40.0%
% Dry Shrinkage: 7.5
Dry M.O.R., psi:* 890
pH: 4.3
C.E.C., meq/100g: 11.5
Soluble sulfur:** Med-High

Cone 5 10
----
Total Shrinkage: 15.5% 17.5%
Absorption: 14.0% 3.5%

P.C.E.: 32

Particle Size, Microns: 20 10 5 2 1 0.5 0.2
97% 95% 90% 80% 70% 56% 31%

*Modulus of Rupture Specimens: De-aired, extruded, 50% ball clay, 50% flint
**Low-trace to 150, Med-150-400, High-450+

Related Information

Links

Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.

Data

Pyrometric Cone Equivalent 32

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy