IXL #39 Clay

Oxide Analysis Formula Tolerance
CaO 9.64% 0.53
K2O 2.28% 0.07
MgO 4.51% 0.34
Na2O 1.08% 0.05
TiO2 0.47% 0.02
Al2O3 10.68% 0.32
SiO2 53.41% 2.73
Fe2O3 4.04% 0.08
LOI 13.12%n/a
Oxide Weight 264.65
Formula Weight 304.62

Notes

A highly calcarious, low temperature, pale red burning clay. The clay portion is mostly illite with some montmorillonite and a fair amount of free silica. Was used in making brick. No longer available.

Related Information

Links

Typecodes Clay Other
Clays that are not kaolins, ball clays or bentonites. For example, stoneware clays are mixtures of all of the above plus quartz, feldspar, mica and other minerals. There are also many clays that have high plasticity like bentonite but are much different mineralogically.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy