Alternate Names: IMCO 800
Description: Smooth plastic red fireclay
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 0.18% | 0.01 | |
| K2O | 1.69% | 0.06 | |
| Na2O | 0.15% | 0.01 | |
| Al2O3 | 28.60% | 1.00 | |
| SiO2 | 53.20% | 3.16 | |
| Fe2O3 | 4.51% | 0.10 | |
| MgO | 0.67% | 0.06 | |
| TiO2 | 1.27% | 0.06 | |
| LOI | 7.30% | n/a | |
| Oxide Weight | 321.94 | ||
| Formula Weight | 347.29 | ||
The manufacturer claims this is a milled and air floated Lincoln fire clay. It is an excellent all purpose clay with high strength and plasticity.
Ground to 200 mesh, this is a refractory plastic smooth tan burning very smooth plastic clay with kaolin-like working properties. Although referred to as a fireclay, it bloats by cone 11. It is yellowish in the raw state.
To formulate a substitute for Newman fireclay we mixed this 50:50 with Carbondale Red and added 15% silica and made a body having a recipe containing 50% Newman. The results showed that this mix has less color than Newman and is quite a bit more vitreous. Much more silica will be needed to cut the maturity and this will result in loss of color making the addition of iron necessary.
Physical data can be found on the link to the product information web page of the manufacturer.

This picture has its own page with more detail, click here to see it.
Cone 10R (bottom) and cone 10, 8, 7 and 6 oxidation.
| Materials |
Imco 400 Fireclay
|
| Materials |
Fireclay
|
| Materials |
Lincoln 8 Clay
|
| Materials |
C-Red Clay
|
| Materials |
Newman Red Clay
|
| URLs |
https://www.clayimco.com/industrial-clays
IMCO information on their mined clays |
| Typecodes |
Fireclay
Fireclays are non-kaolin non-ball clay materials similar to stoneware clays but lacking fluxing oxides. Many fireclays have a PCE of 28 or more. |
| Typecodes |
Refractory
Materials that melt at high temperatures. These are normally used for kiln bricks, furniture, etc. or for ceramics that must withstand high temperatures during service. |
![]() PayPal | No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me. |
| By Tony Hansen Follow me on ![]() | ![]() |
Buy me a coffee and we can talk