1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

Hays Special Clay

Alternate Names: Hays Special Ball Clay

Description: Ball Clay

Oxide Analysis Formula Tolerance
CaO 0.20% 0.01
K2O 0.98% 0.04
MgO 0.34% 0.03
Na2O 0.21% 0.01
TiO2 1.37% 0.07
Al2O3 25.30% 1.00
P2O5 0.07% -
SiO2 60.00% 4.02
Fe2O3 1.30% 0.03
MnO 0.01% -
LOI 10.15%n/a
SO3 0.05%n/a
Oxide Weight 361.96
Formula Weight 403.07

Notes

Relative Viscosity (1.2 Sp. Gr.):* 1.29
Casting Rate: (gms per 15 min/426 cm2):* 208
Water of Plasticity:* 20.6
% Dry Shrinkage:* 4.75
Dry M.O.R., psi:* 447

Cone 04 8 11
----
Fired Shrinkage:* 0.0% 1.5% 2.3%
Absorption:* 22.1% 15.6% 10.6%
M.O.R. psi:* 1930 3420 5349

Thermal Expansion, Cone 8: .475% at 700C
P.C.E.: 31
pH: 5.4
Oil Absorption: 36
Bulk Density, lbs per cubic foot: 35-40
Particle Size, Microns: 20 10 5 2 1 0.5 0.2
95% 90% 81% 60% 42% 25% 5%

*Specimens: De-aired, extruded, 50% ball clay, 50% flint

Related Information

Links

Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy