Fusion Frit FL-31

Alternate Names: Frit FL31

Description: Cadmium frit for cadmium/selenium class colors

Oxide Analysis Formula Tolerance
CaO 0.80% 0.05
K2O 1.50% 0.06
Na2O 9.50% 0.53
CdO 3.70% 0.10
PbO 17.20% 0.27
Al2O3 3.10% 0.11
B2O3 14.80% 0.74
SiO2 47.00% 2.70
ZrO2 0.60% 0.02
Oxide Weight 339.46
Formula Weight 339.46

Related Information

Links

Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Materials Pemco Frit PB-1V48
Typecodes Leaded Frit
Frits can contain 1% or 80% PbO so this category can be misleading, check the chemistry to find out.
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.

Mechanisms

Glaze ColorLead cadmium frits are available as a base to create classic cadmium selenium colors that cannot be easily achieved in other ways. These glazes can be toxic to work with and the glazed ware will likely leach cadmium.
Glaze ColorLead cadmium frits are available as a base to create classic cadmium selenium colors that cannot be easily achieved in other ways. These glazes can be toxic to work with and the glazed ware will likely leach cadmium.
Glaze ColorLead cadmium frits are available as a base to create classic cadmium selenium colors that cannot be easily achieved in other ways. These glazes can be toxic to work with and the glazed ware will likely leach cadmium.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy