Frit A 3021

Alternate Names: Frit A3021

Description: Reimbold & Strick low expansion Ca-B frit

Oxide Analysis Formula Tolerance
CaO 10.00% 1.00
ZrO2 3.00% 0.14
Al2O3 10.00% 0.55
SiO2 51.00% 4.76
B2O3 26.00% 2.10
Oxide Weight 561.00
Formula Weight 561.00

Related Information

A frit manufacturer that used to publish chemistry


This picture has its own page with more detail, click here to see it.

I was impressed with this frit company, Reimbold & Strick. Their frit data was educational, by studying the chemistry of their matte frits, for example, you could see the various mechanisms that produce the effect. But, it is no longer available. However, with a little determination you could likely find the pages at the internet archive (see link below).

Links

Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.

Data

Co-efficient of Linear Expansion 42 X 10-7 (20-400C)
Frit Softening Point 710C
Glass Transition Temperature 650C

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy