Alternate Names: Fertogel Attapulgite

Description: Hydrous magnesium aluminum silicate clay

Oxide Analysis Formula Tolerance
SiO2 57.10% 2.90
Al2O3 10.70% 0.32
MgO 11.10% 0.84
CaO 2.30% 0.12
Fe2O3 4.20% 0.08
K2O 0.80% 0.03
Na2O 0.20% 0.01
TiO2 0.50% 0.02
LOI 13.00%n/a
Oxide Weight 264.82
Formula Weight 304.39

Notes

A ground attapulgite clay, was primarily used as a suspending agent in liquid fertilizers. Current status is unknown.

Related Information

Links

Typecodes Clay Other
Clays that are not kaolins, ball clays or bentonites. For example, stoneware clays are mixtures of all of the above plus quartz, feldspar, mica and other minerals. There are also many clays that have high plasticity like bentonite but are much different mineralogically.

Data

Sieve Analysis Wet +200 mesh: 8%
Bulk Density lbs/cu. ft. (Packed) 43 loose, 55 packed
Density (Specific Gravity) 2.35
pH for dry powder 10

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy