Ferro Frit 4110

Alternate Names: Frit KFG 4110, Frit DA4110

Description: Leadless high expansion high alkali frit, formerly Frit 3110

Oxide Analysis Formula Tolerance
CaO 6.13% 0.29
K2O 2.54% 0.07
Na2O 15.31% 0.64
B2O3 2.68% 0.10
Al2O3 4.20% 0.11
SiO2 69.15% 3.00
Oxide Weight 261.01
Formula Weight 261.01

Notes

Good for copper blues and manganese purples.
Very similar but not identical to Ferro Frit 3110.
The data sheet at Walker Ceramics 2015 shows a little less SiO2 than this one.

Related Information

Links

Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Materials Ferro Frit 3110
High sodium, high thermal expansion low boron frit. A super-feldspar in clay bodies. Melts at very low temperatures. Useful to make crackle glazes.
Materials Frit 1078
Materials Keramikos Fritte 31.10
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.

Data

Co-efficient of Linear Expansion 8.50
Frit Softening Point 575C
Frit Melting Range (C) 1000-1060C
Glass Transition Temperature 531C

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy