1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

Ferro Frit 3435

Description: Low lead low alumina calcium borosilicate frit

Oxide Analysis Formula Tolerance
CaO 7.30% 0.39
K2O 1.40% 0.04
Na2O 4.30% 0.21
PbO 25.90% 0.35
B2O3 16.30% 0.71
Al2O3 2.20% 0.07
SiO2 42.60% 2.15
Oxide Weight 302.68
Formula Weight 302.68

Related Information

Links

Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Materials Hommel Frit 536
Typecodes Leaded Frit
Frits can contain 1% or 80% PbO so this category can be misleading, check the chemistry to find out.
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.

Data

Co-efficient of Linear Expansion 7.50
Frit Melting Range (C) 1300F

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy