F. C. Kaolin

Description: COARSE GRAINED GEORGIA KAOLIN

Oxide Analysis Formula Tolerance
CaO 0.04% -
K2O 0.11% -
MgO 0.02% -
Na2O 0.02% -
TiO2 1.77% 0.06
Al2O3 38.21% 1.00
SiO2 45.16% 2.01
Fe2O3 0.36% 0.01
LOI 13.51%n/a
Oxide Weight 228.75
Formula Weight 264.48

Notes

Originally referred to as FAST CAST, F.C. Clay is a secondary, coarse grained Georgia Clay with a particle size distribution approaching that of fractional clay. The chemical analysis is close to that of theoretical kaolinite. Uniformity, excellent color, low C.E.C., surface area, ease of dispersion and coarseness are notable characteristics. It is available in lump, dried, airfloated and slurry forms.

PCE: 34
+325 Residue (%): 1
pH: 4.5-6.5
C.E.C.: 2.00
Specific Gravity: 2.62
Casting Rate gms/30'(Bariod): 120
Bulk Density: 30#/c. ft.

% finer than 10 microns: 96
10 microns: 87
5 microns: 71
2 microns: 49
1 micron: 37
0.5 micron: 24

Median particle diameter (microns): 2.0
Specific surface area (sq. meters/gram): 10.0

Related Information

Links

Materials Kaolin
The purest of all clays in nature. Kaolins are used in porcelains and stonewares to impart whiteness, in glazes to supply Al2O3 and to suspend slurries.
Typecodes Kaolin
Pure clay mineral, there are many brand names of varying purity and iron content.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy