F-1 Clay

Description: CLAY

Oxide Analysis Formula Tolerance
CaO 0.34% 0.03
K2O 1.65% 0.08
MgO 1.01% 0.11
Na2O 0.18% 0.01
TiO2 1.29% 0.07
Al2O3 22.67% 1.00
SiO2 60.93% 4.56
Fe2O3 3.44% 0.10
LOI 8.50%n/a
Oxide Weight 411.73
Formula Weight 449.98

Notes

Crude Color: Brown
Dry M.O.R. (psi 50% clay/50% flint, cast bars): 1260
Wet Sieve Residue, +200 mesh (%): 0.20
Water of Plasticity (%): 40
Oil Absoprtion: 46.0
Solubles Sulfates (ppm): 252
Filtration (ml): 17
Specific Surface Area (sq meters per gram): 25.46
CEC/MBI (meq/100 ml): 17
pH: 6.6
Particle Size (% less than):
5 micron: 80
1 micron: 39
.5 micron: 26
Median Paricle Diameter (Micron): 1.66

Firing Shrinkage (%) Cone 04: 7.4 Cone 3: 8.1
Absorption (%) 10.1 5.6

Related Information

Links

Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy