Black Charm Clay

Alternate Names: Ball Charm Ball Clay

Description: Ball Clay

Oxide Analysis Formula Tolerance
CaO 0.33% 0.03
K2O 1.34% 0.06
MgO 0.21% 0.02
Na2O 0.32% 0.02
TiO2 0.20% 0.01
Al2O3 22.66% 1.00
P2O5 0.04% -
SiO2 62.96% 4.72
Fe2O3 1.53% 0.04
MnO 0.05% -
LOI 10.52%n/a
SO3 0.11%n/a
Oxide Weight 403.50
Formula Weight 451.49

Notes

A coarse-grained engineered blend offering a high degree of moisture retention, plasticity, and naturally occurring organics. Ideally suited for a variety of bonding applications.

Relative Viscosity (1.2 Sp. Gr.):* 1.23
Casting Rate: (gms per 15 min/426 cm2):* 165
Water of Plasticity:* 26.4
% Dry Shrinkage:* 5.55
Dry M.O.R., psi:* 496

Cone 04 8 11
----
Fired Shrinkage:* 0.4% 1.5% 2.5%
Absorption:* 21.0% 18.3% 14.8%
M.O.R. psi:* 620 1830 4050

Thermal Expansion, Cone 8: .495% at 700C
P.C.E.: 29
pH: 4.6
Oil Absorption: 32
Bulk Density, lbs per cubic foot: 35-39
Particle Size, Microns: 20 10 5 2 1 0.5 0.2
92% 81% 65% 45% 31% 16% 5%

*Specimens: De-aired, extruded, 50% ball clay, 50% flint

Related Information

Links

Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.

Data

Pyrometric Cone Equivalent 29

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy