Oxide Analysis Formula Tolerance
SiO2 56.00% 3.22 1
Al2O3 29.50% 1.00 1.5
Fe2O3 0.65% 0.01 .05
TiO2 0.75% 0.03 .25
MgO 0.50% 0.04 .1
CaO 0.40% 0.02 .1
Na2O 0.80% 0.04 .2
K2O 0.50% 0.02 .25
LOI 12.00%n/a
Oxide Weight 308.07
Formula Weight 350.08

Notes

Very plastic ball clay from India. Somewhat thixotropic in slurries.

Colour: White
Fired Colour: Creamish/Off White
Plasticity: 30%
Slaking: Moderate
Residue Over 44 Microns: 0.5-1.5
Particle Size > 2 Micron: 30-34
Particle Size > 10 Micron: 9-13
% Dry Shrinkage: 4-6
% Fired Shrinkage: 8-10
% Total Shrinkage: 12-14
Pyrometric Cone Equivalent: 28-30

Related Information

Links

Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy