Bell Gray Ball Clay

Description: Legacy ball clay

Oxide Analysis Formula Tolerance
CaO 0.30% 0.02
MgO 0.30% 0.03
K2O 0.45% 0.02
Na2O 0.45% 0.02
TiO2 1.60% 0.07
Al2O3 30.22% 1.00
SiO2 55.51% 3.12
Fe2O3 0.98% 0.02
Cl 10.19%n/a
Oxide Weight 303.13
Formula Weight 337.52

Related Information

Links

Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.

Data

% < 0.5 microns 56.0%
Drying Shrinkage 8.1
Water absorption 7.0% at cone 9
Dry M.O.R. (50% Silica) 440 psi
Firing Shrinkage 9.9% at cone 9

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy