1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

Bandy Tan

Alternate Names: Bandy Tan Ball Clay

Description: Ball clay

Oxide Analysis Formula Tolerance
CaO 0.32% 0.02
K2O 1.64% 0.07
MgO 0.58% 0.06
Na2O 0.36% 0.02
TiO2 1.26% 0.07
Al2O3 24.38% 1.00
P2O5 0.03% -
SiO2 61.21% 4.26
Fe2O3 1.20% 0.03
MnO 0.01% -
LOI 8.67%n/a
SO3 0.09%n/a
Oxide Weight 380.68
Formula Weight 417.23

Notes

Relative Viscosity (1.2 Sp. Gr.):* 1.2
Casting Rate: (gms per 15 min/426 cm2):* 157
Water of Plasticity:* 27.1
% Dry Shrinkage:* 5.1
Dry M.O.R., psi:* 228

Cone 04 8 11
----
Fired Shrinkage:* 0.4% 3.2% 6.4%
Absorption:* 21.3% 13.8% 5.9%
M.O.R. psi:* 745 2910 5680

Thermal Expansion, Cone 8: .335% at 700C
P.C.E.: 30
pH: 5.5
Oil Absorption: 34
Bulk Density, lbs per cubic foot: 37-45
Particle Size, Microns: 20 10 5 2 1 0.5 0.2
95% 85% 66% 42% 26% 15% 3%

*Specimens: De-aired, extruded, 50% ball clay, 50% flint

Related Information

Links

Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.

Data

Frit Softening Point 30 PCE

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy