98 Mix

Description: Low temperature very plastic iron stained clay

Oxide Analysis Formula Tolerance
Al2O3 13.90% 1.29 13.9
CaO 0.70% 0.12
Fe2O3 2.80% 0.17
K2O 3.00% 0.30
MgO 1.00% 0.24
Na2O 2.20% 0.34
P2O5 0.10% 0.01
SiO2 69.30% 10.95
TiO2 0.60% 0.07
LOI 5.20%n/a
Oxide Weight 888.66
Formula Weight 937.40

Notes

An highly plastic red burning fine-grained material from the Elkwater area in southern Alberta. It was used in brick and pipe manufacture by I-XL Industries and in pottery clay bodies by Plainsman Clays. This was a successor to 45R.

Loring Labs analysis 2006 showed 15.6 Al2O3, 3.9 Fe2O3, 4.9 SO3, 64.9 SiO2, 3.4 LOI.

Related Information

Links

Typecodes Clay Other
Clays that are not kaolins, ball clays or bentonites. For example, stoneware clays are mixtures of all of the above plus quartz, feldspar, mica and other minerals. There are also many clays that have high plasticity like bentonite but are much different mineralogically.
Materials Blue Grey Plastic
Materials IXL 45D
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy