L-1 Ball Clay

Description: Tennessee Ball Clay

Oxide Analysis Formula Tolerance
CaO 0.50% 0.04
K2O 1.40% 0.07
MgO 0.50% 0.06
Na2O 0.20% 0.02
TiO2 1.20% 0.07
Al2O3 21.60% 1.00
SiO2 64.40% 5.06
Fe2O3 1.00% 0.03
LOI 9.20%n/a
Oxide Weight 428.78
Formula Weight 472.22

Notes

A coarse to intermediate-grained, high organic Ball Clay. The high organic content provides additional plasticity, making L-1 ideal for casting or plastic formed bodies. Industry applications include sanitaryware, dinnerware and artware.

Physical Properties
===================
Water of Plasticity*: 37.0%
% Dry Shrinkage*: 6.5
Dry M.O.R., psi:* 825
pH: 4.4
C.E.C., meq/100g: 11.0
Specific Surface Area, sq metre/g: 24.4
Soluble sulfur+: Low

P.C.E.: 32

Particle Size, Microns: 20 10 5 2 1 0.5 0.2
(% finer than) 99% 97% 93% 81% 72% 56% 35%

Fired Properties
================
Cone 5 10
----
Total Shrinkage: 13.0% 14.5%
Absorption: 10.0% 1.0%

Shipped from Mayfield, KY

------------------
*Extruded, 50% ball clay, 50% flint
+Low-trace to 150, Med-150-400, High-450+
**50% Clay, 50% Nepheline Syenite

Related Information

Links

Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.