KTS-Classic

Description: Tennessee Ball Clay

Oxide Analysis Formula Tolerance
CaO 0.30% 0.02
K2O 1.40% 0.06
MgO 0.50% 0.05
Na2O 0.20% 0.01
TiO2 1.40% 0.07
Al2O3 24.60% 1.00
SiO2 61.10% 4.22
Fe2O3 1.00% 0.03
LOI 9.50%n/a
Oxide Weight 375.24
Formula Weight 414.63

Notes

A combination of Kentucky and Tennessee Ball Clays with very good overall plasticity and strength. KTS-Classic can be used in casting or plastic formed bodies. It is also supplied in a clay-water slurry form for use by the sanitaryware and artware industries.

Physical Properties
===================
Water of Plasticity*: 37.0%
% Dry Shrinkage*: 6.5
Dry M.O.R., psi:* 825
pH: 4.4
C.E.C., meq/100g: 11.0
Specific Surface Area, sq metre/g: 24.4
Soluble sulfur+: Low

P.C.E.: 32

Particle Size, Microns: 20 10 5 2 1 0.5 0.2
(% finer than) 99% 97% 93% 81% 72% 56% 35%

Fired Properties
================
Cone 5 10
----
Total Shrinkage: 13.0% 14.5%
Absorption: 10.0% 1.0%

Shipped from Mayfield, KY

------------------
*Extruded, 50% ball clay, 50% flint
+Low-trace to 150, Med-150-400, High-450+
**50% Clay, 50% Nepheline Syenite

Related Information

Links

Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy