K-200 Feldspar

Alternate Names: K200 Feldspar

Description: POTASSIUM/SODIUM/CALCIUM FELDSPAR

Oxide Analysis Formula Tolerance
CaO 0.18% 0.02
K2O 10.13% 0.65
Na2O 3.36% 0.33
Al2O3 17.84% 1.06
SiO2 67.99% 6.86
Fe2O3 0.08% -
LOI 0.31%n/a
Oxide Weight 603.74
Formula Weight 605.61

Notes

K-200 is a high quality feldspar ground to 200 mesh for ceramic applications. It has one of the highest potassium contents of any spar. Carefully beneficiated and controlled for quality, K-200 offers high potash content and low iron oxide per unit of alumina.

Sieve Analysis (Cum):
+200 mesh: 0.3%
+325 mesh: 3.2%

Average Particle Size: 10.1 microns
Specific Surface Area: 1.88 square meters per gram
Bulk Density: 62 lbs/cu ft loose, 74 packed

Related Information

Links

Typecodes Feldspar
The most common source of fluxes for high and medium temperature glazes and bodies.